abide by the contract", conforms to the market requirement, joins in the market competition by its high quality as well as provides more comprehensive and excellent service for clients to let them become big winner. The pursue of the company, is the clients' satisfaction for Massive Selection for Titanium alloy 6Al-4V ELI UNS R56401 Factory for South Korea, Welcome to build the well and long standing business relationships with our company to create a glorious future together .customers' satisfaction is our eternal pursuit
HY Titanium 6-4 ELI Material grades and equivalents
6-4 ELI Titanium, 6-4 ELI, UNS R56401
Introduction
Low interstitial version of HY Titanium 6-4 ELI, for maximum toughness. Preferred for marine and cryogenic applications. This grade is normally used in the annealed condition. HY Titanium 6-4 ELI is the preferred choice for the medical implant field.
Stress relief 900-1200°F 1 to 4 hours, air cool. Duplex anneal, bar and forgings: Solution anneal 50-100°F below the beta transus, hold 1 hour minimum, air cool. Then reheat within the range 1300-1400°F, hold 1 hour minimum, air cool. Stress – relief annealing is performed after welding.
Chemistry Composition
Al |
V |
Fe |
O |
C |
N |
H |
Y |
Others, |
Others, |
Ti |
|
MIN |
5.5 |
3.5 |
– |
– |
– |
– |
– |
– |
– |
– |
– |
MAX |
6.5 |
4.5 |
0.25 |
0.13 |
0.08 |
0.03 |
0.0125 |
0.005 |
0.1 |
0.4 |
Balance |
Features
Resistant to bodily fluidsResistant to a variety of corrosive environmentsFreedom from chloride stress corrosion crackingGood strength and toughness over a wide temperature rangeHigh resistance to erosion corrosion and corrosion fatigueUseful resistance to dry chlorine, fluorine, hydrogen chloride and hydrogen fluoride gases
Applications
Medical and dental implantsCryogenicsAerospaceChemical processing
Physical Properties
Density: 0.160 lb/in3
Melting Range: 2370 – 2460°F
Beta Transus: 91790+25°F
Minimum Tensile Properties, AMS 4919, Duplex Annealed
Temperature, °F |
68-212 |
68-600 |
68-1000 |
68-1200 |
68-1500 |
Coefficient* of Thermal Expansion, in/in°F x 10-6 |
9.18 |
9.54 |
10.08 |
10.44 |
10.8 |
Mechanical Properties
Typical hardness Rockwell: C 30-34 Specific minimums, AMS 4931, bar and forging
Representative Tensile Properties, Sheet
Diameter, in |
< 3.0 |
< 3.0 < 4.0 |
< 4.0) < 6.0 |
Tensile Strength, ksi |
125 |
123 |
120 |
0.2 % Yield Strength, ksi |
115 |
110 |
110 |
Elongation, % *L (**ST) |
10 (8) |
10 (8) |
8 (8) |
Reduction of Area, % *L (**ST) |
25 (–) |
20 (15) |
15 (15) |
* Longitudinal ** Short Transverse
Typical Elevated temperature Properties
Temperature, °F |
93 (200) |
149 (300) |
204 (400) |
260 (500) |
Ultimate Tensile Strength, ksi |
843.3 (121) |
772.2 (112) |
723.9 (105) |
657.7 (98) |
0.2 % Yield Strength, ksi |
710.2 (103) |
641.2 (93) |
586.1 (85) |
531.0 (77) |
Elongation, % |
13 |
15 |
16 |
16 |
Regular shape for all kinds of alloys | |||
Form | Specification | Supply Form | Others |
Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
Forged barΦ26-245mm,Length≤4000mm | |||
Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
Straight WireΦ1.6mm-4.0mm | |||
Welding rodΦ1.2mm-4.0mm | |||
Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
I am earning my own wedding day band from Inconel X-750 just to be diverse. The material is a agony to do the job with thanks to the superior nickel/chromium articles. The lathe is a LeBlond “dual generate” with an Aloris-copy device article. I built an adapter for the one.25″ boring bar socket to sleeve it down to a 5/8″ side-lock drill shank. I utilised an indicator to sweep the device holder, inserting it instantly on center. The drill is a Seco CrownLoc As well as with .625″ tip, running at around 80sfm, hand feed with plenty of stress, and drenched in reducing oil (not demonstrated in pic). Chips had been astonishingly limited of course, I had to withdrawal the device numerous moments to eliminate chips, due to the fact they weren’t becoming flushed by coolant.
A nitinol wire/form memory alloy inchworm that walks across a table employing only warmth. The warmth is supplied by electrical existing heating up the skinny nitinol wire, causing it to return to its remembered form, a compressed coil in this scenario. A V-formed spring returns it to the commencing form.
Guidance RimstarOrg on Patreon https://www.patreon.com/user?u=680159
Subscribe for new films every single week http://www.youtube.com/user/rimstarorg?sub_affirmation=1
Go to the principal channel webpage below https://youtube.com/rimstarorg
See also:
How to Make Nitinol Wire Inchworm (Shape Memory Alloy)
https://www.youtube.com/look at?v=getfzfZJjHM
Nitinol Wire – How to Use it
https://www.youtube.com/look at?v=4Yi4epJ83EE
How a Rocket Performs/Earth to Area Eg SpaceX Falcon 9 and Dragon
https://www.youtube.com/look at?v=L0AMQ6kRNMA
My webpage about this nitinol wire inchworm:
http://rimstar.org/science_electronics_tasks/nitinol_wire_inchworm_form_memory_alloy_handmade.htm
Adhere to at the rear of-the-scenes on:
Twitter https://twitter.com/#!/RimStarz
Google+ https://additionally.google.com/116395125136223897621
Fb https://www.fb.com/rimstarorg
http://rimstar.org
The inspiration came from this one:
https://www.youtube.com/look at?v=DW4WaTmoZ3c
Essence – audio by audionautix.com