15 Years Factory Titanium alloy 6Al-4V ELI UNS R56401 Wholesale to Lithuania
We are proud of the high customer satisfaction and wide acceptance due to our persistent pursuit of high quality both on product and service for 15 Years Factory Titanium alloy 6Al-4V ELI UNS R56401 Wholesale to Lithuania, We welcome customers, business associations and friends from all parts of the world to contact us and seek cooperation for mutual benefits.
HY Titanium 6-4 ELI Material grades and equivalents
6-4 ELI Titanium, 6-4 ELI, UNS R56401
Introduction
Low interstitial version of HY Titanium 6-4 ELI, for maximum toughness. Preferred for marine and cryogenic applications. This grade is normally used in the annealed condition. HY Titanium 6-4 ELI is the preferred choice for the medical implant field.
Stress relief 900-1200°F 1 to 4 hours, air cool. Duplex anneal, bar and forgings: Solution anneal 50-100°F below the beta transus, hold 1 hour minimum, air cool. Then reheat within the range 1300-1400°F, hold 1 hour minimum, air cool. Stress – relief annealing is performed after welding.
Chemistry Composition
|
|
Al |
V |
Fe |
O |
C |
N |
H |
Y |
Others, |
Others, |
Ti |
|
MIN |
5.5 |
3.5 |
– |
– |
– |
– |
– |
– |
– |
– |
– |
|
MAX |
6.5 |
4.5 |
0.25 |
0.13 |
0.08 |
0.03 |
0.0125 |
0.005 |
0.1 |
0.4 |
Balance |
Features
- Resistant to bodily fluids
- Resistant to a variety of corrosive environments
- Freedom from chloride stress corrosion cracking
- Good strength and toughness over a wide temperature range
- High resistance to erosion corrosion and corrosion fatigue
- Useful resistance to dry chlorine, fluorine, hydrogen chloride and hydrogen fluoride gases
Applications
- Medical and dental implants
- Cryogenics
- Aerospace
- Chemical processing
Physical Properties
Density: 0.160 lb/in3
Melting Range: 2370 – 2460°F
Beta Transus: 91790+25°F
Minimum Tensile Properties, AMS 4919, Duplex Annealed
|
Temperature, °F |
68-212 |
68-600 |
68-1000 |
68-1200 |
68-1500 |
|
Coefficient* of Thermal Expansion, in/in°F x 10-6 |
9.18 |
9.54 |
10.08 |
10.44 |
10.8 |
Mechanical Properties
Typical hardness Rockwell: C 30-34 Specific minimums, AMS 4931, bar and forging
Representative Tensile Properties, Sheet
|
Diameter, in |
< 3.0 |
< 3.0 < 4.0 |
< 4.0) < 6.0 |
|
Tensile Strength, ksi |
125 |
123 |
120 |
|
0.2 % Yield Strength, ksi |
115 |
110 |
110 |
|
Elongation, % *L (**ST) |
10 (8) |
10 (8) |
8 (8) |
|
Reduction of Area, % *L (**ST) |
25 (–) |
20 (15) |
15 (15) |
* Longitudinal ** Short Transverse
Typical Elevated temperature Properties
|
Temperature, °F |
93 (200) |
149 (300) |
204 (400) |
260 (500) |
|
Ultimate Tensile Strength, ksi |
843.3 (121) |
772.2 (112) |
723.9 (105) |
657.7 (98) |
|
0.2 % Yield Strength, ksi |
710.2 (103) |
641.2 (93) |
586.1 (85) |
531.0 (77) |
|
Elongation, % |
13 |
15 |
16 |
16 |
| Regular shape for all kinds of alloys | |||
| Form | Specification | Supply Form | Others |
| Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
| Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
| Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
| Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
| Forged barΦ26-245mm,Length≤4000mm | |||
| Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
| Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
| Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
| Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
| Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
| Straight WireΦ1.6mm-4.0mm | |||
| Welding rodΦ1.2mm-4.0mm | |||
| Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
This is our 4000 watt Co2 laser slicing process. We can cut Stainless Steel and alloys to .five hundred”, Steel and metal alloys to .750″ and aluminum to .375″. Equally our devices have big bed dimensions, just one is sixty” x 120″ and the 3000 watt is seventy eight” x 157″. Equally devices have automatic loading and shuttle tables for prototyping to manufacturing.
Melting down 1 gram bars of Silver, Copper, Nickel and Brass with hydrogen and oxygen. Brass is previously an alloy of copper and zinc, and did not soften down effortless as a I figured out from my Brass, Guide and Gunpowder video clip. I then blend the a few workable metals Silver, copper and nickel to generate…….Silvcopickel
SUBSCRIBE: http://comprehensive.sc/1bnslc9
Facebook: http://comprehensive.sc/1dT2aaM
RHNB Vs. Watermelon – http://comprehensive.sc/1bns60F
RHNB Vs. Jello – http://comprehensive.s/1bns0WF RHNB Vs. Elmers Glue – http://comprehensive.sc/1dT1TEM
RHNB Entire Playlist – http://comprehensive.sc/1dT1WjP -Want to ship an object / materials / substance to be RHNB’d or HHO’d? Send Here with a comprehensive credit of your donation! PO Box 21 96 Seymour St. Tonawanda NY 14150 Usa