Factory making Iron alloy Stainless Steel 17-4PH for Bangladesh Importers
We always think and practice corresponding to the change of circumstance, and grow up. We aim at the achievement of a richer mind and body and the living for Factory making Iron alloy Stainless Steel 17-4PH for Bangladesh Importers, we have built a reliable reputation among many customers. Quality&customer first are always our constant pursuit. We spare no efforts to make better products. Look forward to long-term cooperation and mutual benefits!
|
HY 17-4PH Material grades and equivalents |
|
||
|
UNS |
AISI/ASTM |
JIS |
W.Nr |
|
S17400 |
630,17-4PH |
SUS630 |
1.4542 |
|
HY 17-4PH Chemical composition: |
|
|
|
|
|
|
|
|
|||
|
Alloy |
% |
Ni |
Cr |
Fe |
C |
Mn |
Si |
S |
Cu |
Nb |
P |
|
HY 17-4PH |
Min. |
3 |
15.5 |
balance |
|
|
|
|
3 |
0.15 |
|
|
Max. |
5 |
17.5 |
0.07 |
1 |
1 |
0.03 |
5 |
0.45 |
0.035 |
||
|
HY 17-4PH Physical properties |
||
|
Density |
7.78/cm3 |
|
|
Melting point |
1400-1440 °C |
|
|
HY 17-4PH Minimum mechanical properties in the room temperature |
||||||
|
Status |
Tensile strength |
Yield strength |
Elongation |
HRC(HBS) |
|
|
|
Rm N/mm² |
Rp0.2 N/mm² |
A5 % |
|
|
||
|
480°C age |
≥1310 |
≥1180 |
≥10 |
≥40 |
|
|
|
550°C Age |
≥1060 |
≥1000 |
≥12 |
≥35 |
|
|
|
580°C age |
≥1000 |
≥865 |
≥13 |
≥31 |
|
|
|
620°C age |
≥930 |
≥325 |
≥16 |
≥28 |
|
|
|
HY 17-4PH Characteristic: |
|
|
|
|
|
||
|
High strength and hardness, good welding performance and corrosion resistance |
|||||||
|
|
|
|
|
|
|
|
|
|
HY 17-4PH Application range and field: |
|
|
|
|
|||
|
Used in components with high strength and corroson resistance |
|
||||||
| Regular shape for all kinds of alloys |
|||
| Form | Specification | Supply Form | Others |
| Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
| Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
| Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
| Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
| Forged barΦ26-245mm,Length≤4000mm | |||
| Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
| Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
| Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
| Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
| Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
| Straight WireΦ1.6mm-4.0mm | |||
| Welding rodΦ1.2mm-4.0mm | |||
| Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
This is our 4000 watt Co2 laser slicing process. We can cut Stainless Steel and alloys to .five hundred”, Steel and metal alloys to .750″ and aluminum to .375″. Equally our devices have big bed dimensions, just one is sixty” x 120″ and the 3000 watt is seventy eight” x 157″. Equally devices have automatic loading and shuttle tables for prototyping to manufacturing.
Supplier foil、strip、sheet、coil、plate、wire、rod、bar、tube、pipe、flat ribbon、Profiled wire…
BuildingNo.1,3rd Industrial District XiTou Village SongGang Town Bao’An District ShenZhen Town GuangDong Province China