Our company promises all users of the first-class products and the most satisfying post-sale service. We warmly welcome our regular and new customers to join us for Factory Supplier for Titanium alloy 6Al-4V ELI UNS R56401 Wholesale to Germany, Competitive price with high quality and satisfying service make us earned more customers.we wish to work with you and seek common development.
HY Titanium 6-4 ELI Material grades and equivalents
6-4 ELI Titanium, 6-4 ELI, UNS R56401
Introduction
Low interstitial version of HY Titanium 6-4 ELI, for maximum toughness. Preferred for marine and cryogenic applications. This grade is normally used in the annealed condition. HY Titanium 6-4 ELI is the preferred choice for the medical implant field.
Stress relief 900-1200°F 1 to 4 hours, air cool. Duplex anneal, bar and forgings: Solution anneal 50-100°F below the beta transus, hold 1 hour minimum, air cool. Then reheat within the range 1300-1400°F, hold 1 hour minimum, air cool. Stress – relief annealing is performed after welding.
Chemistry Composition
|
Al |
V |
Fe |
O |
C |
N |
H |
Y |
Others, |
Others, |
Ti |
|
|
MIN |
5.5 |
3.5 |
– |
– |
– |
– |
– |
– |
– |
– |
– |
|
MAX |
6.5 |
4.5 |
0.25 |
0.13 |
0.08 |
0.03 |
0.0125 |
0.005 |
0.1 |
0.4 |
Balance |
Features
Resistant to bodily fluidsResistant to a variety of corrosive environmentsFreedom from chloride stress corrosion crackingGood strength and toughness over a wide temperature rangeHigh resistance to erosion corrosion and corrosion fatigueUseful resistance to dry chlorine, fluorine, hydrogen chloride and hydrogen fluoride gases
Applications
Medical and dental implantsCryogenicsAerospaceChemical processing
Physical Properties
Density: 0.160 lb/in3
Melting Range: 2370 – 2460°F
Beta Transus: 91790+25°F
Minimum Tensile Properties, AMS 4919, Duplex Annealed
|
Temperature, °F |
68-212 |
68-600 |
68-1000 |
68-1200 |
68-1500 |
|
Coefficient* of Thermal Expansion, in/in°F x 10-6 |
9.18 |
9.54 |
10.08 |
10.44 |
10.8 |
Mechanical Properties
Typical hardness Rockwell: C 30-34 Specific minimums, AMS 4931, bar and forging
Representative Tensile Properties, Sheet
|
Diameter, in |
< 3.0 |
< 3.0 < 4.0 |
< 4.0) < 6.0 |
|
Tensile Strength, ksi |
125 |
123 |
120 |
|
0.2 % Yield Strength, ksi |
115 |
110 |
110 |
|
Elongation, % *L (**ST) |
10 (8) |
10 (8) |
8 (8) |
|
Reduction of Area, % *L (**ST) |
25 (–) |
20 (15) |
15 (15) |
* Longitudinal ** Short Transverse
Typical Elevated temperature Properties
|
Temperature, °F |
93 (200) |
149 (300) |
204 (400) |
260 (500) |
|
Ultimate Tensile Strength, ksi |
843.3 (121) |
772.2 (112) |
723.9 (105) |
657.7 (98) |
|
0.2 % Yield Strength, ksi |
710.2 (103) |
641.2 (93) |
586.1 (85) |
531.0 (77) |
|
Elongation, % |
13 |
15 |
16 |
16 |
| Regular shape for all kinds of alloys | |||
| Form | Specification | Supply Form | Others |
| Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
| Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
| Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
| Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
| Forged barΦ26-245mm,Length≤4000mm | |||
| Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
| Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
| Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
| Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
| Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
| Straight WireΦ1.6mm-4.0mm | |||
| Welding rodΦ1.2mm-4.0mm | |||
| Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
NEW 2016 Chrysler three hundred S Alloy Edition Sedan with a Gloss Black Paint finish. AWD that seats five with a three.two L V-six engine and an eight velocity computerized transmission. 19″ alluminum alloy rims with Michelin Primacy MXM4 tires. This sedan will come thoroughly loaded with keyless entry, distant get started, power locks, home windows, mirrors, Beats by Dre audio system, AM/FM, Sirius Sat radio, Lcd display screen in the entrance with back up digicam, leather all over with heated entrance and rear seats and so significantly a lot more. Come check out it out at Ponoka Chrysler and see what else it has to present, we are located on the south conclusion of Ponoka just off of HWY 2A.
Stock# 16C37644
Sarah Johnson,
Ponoka Chrysler
6510 39th Ave Ponoka, AB T4J 1J8
Toll Cost-free: 1(800) 265-6851
Cellphone: (403) 783-5383
Fax: (403) 783-8140
E-mail: sjohnson@ponokachrysler.com
Like us on Fb- https://www.facebook.com/PonokaChrysler/
Abide by us on Instargram- https://www.instagram.com/ponokadodge/
Abide by us on Twitter- https://twitter.com/PonokaDodgeRam
Abide by us on Pintrest- https://www.pinterest.com/ponokachrysler/
Check out additional TIG Welding Video clips from Weld.com:
http://www.weld.com/index.php/Mr-Tig-Blog/
Subscribe on YouTube and Never ever Miss a Video!
http://www.youtube.com/channel/UCM0kHJXSHR1k1wtLuliKmHg?sub_confirmation=one
Pay a visit to the Welding Discussion board to Carry on the Dialogue and Compete in Month to month Contests!
http://www.weld.com/index.php/Weekend-Warrior-Welding-Discussion board/groups.html
Fb: https://www.fb.com/WeldDotCom
Twitter: https://twitter.com/WeldDotCom
—————————————————————————–
Weld.com welding films are a collection of welding displays that are loaded with welding strategies, tricks and hints that will support you drop that perfect bead each individual time! Whether you are making an attempt to become far better in the locations of TIG Welding, MIG Welding, Adhere Welding or Slicing Weld.com has what you will need. All films are shot from “guiding the hood” so you can get the welders standpoint. In addition to exhibiting you how to weld, many periods we will clearly show you popular issues and how to steer clear of them.
New episodes each individual Friday!
Early launch on the discussion board!