New Fashion Design for Titanium alloy 6Al-4V STA UNS R56400 Factory for Rwanda
Dedicated to strict quality control and thoughtful customer service, our experienced staff members are always available to discuss your requirements and ensure full customer satisfaction for New Fashion Design for Titanium alloy 6Al-4V STA UNS R56400 Factory for Rwanda, With the aim of "compete with good quality and develop with creativity" and the service principle of "take customers' demand as orientation", we will earnestly provide qualified products and good service for domestic and international customers.
HY Titanium 6-4 STA Material grades and equivalents
6-4 STA Titanium, 6-4 STA, Ti 6-4 STA, UNS R56400
Introduction
HY Titanium 6-4 STA (Solution Treated and Aged) is a modified version of Ti 6Al-4V. It is heat treated for high strength in sections under 4″ thick. Ti-6Al-4V has excellent hardenability in sections up to 1″ thick with strengths as high as 165 ksi.
For maximum strength: solution-treated and aged (STA) condition is: For sheet, 1675-1725°F 5 to 25 minutes, water quench. Age 975°F 4 to 6 hours, air cool. For bars and forgings, 1675-1725°F 1 hour, water quench. Age 975-1025°F 4 to 8 hours, air cool.
HY Titanium 6-4 STA is resistant to general corrosion but may be quickly attacked by environments that cause breakdown of the protective oxide. These include hydrofluoric (HF), hydrochloric (HCl), sulfuric and phosphoric acids. Inhibitors may help for the last three but not for HF. Ti 6Al-4V STA resists attack by pure hydrocarbons, and most chlorinated and fluorinated hydrocarbons (provided water has not caused formation of small amounts of HCl and HF).
Chemistry Composition
|
Al |
V |
C |
N |
O |
H |
Fe |
Y |
Others, |
Others, |
Ti |
|
|
MIN |
5.5 |
3.5 |
– |
– |
– |
– |
– |
– |
– |
– |
– |
|
MAX |
6.75 |
4.5 |
0.08 |
0.05 |
0.2 |
0.0125 |
0.3 |
0.005 |
0.1 |
0.4 |
Balance |
Features
High strength to 750°FExcellent general corrosion resistanceHigh strength-to-weight ratio
Applications
Aerospace, turbine engine and airframe applicationsFastenersMedical and dental implantsHigh performance Automotive
Physical Properties
Density: 0.160 lb/inch3
Melting Range: 2920 – 3020°F
Beta Transus: 1825± 25°F
|
Temperature, °F |
70 |
200 |
400 |
600 |
|
Coefficient of Thermal Expansion, in/in°F x 10-6 |
- |
5.3 |
5.4 |
5.5 |
|
Thermal Conductivity, |
4.0 |
4.3 |
5.2 |
6.1 |
|
Modulus of Elasticity, |
16.7 |
16.0 |
15.0 |
14.0 |
Mechanical Properties
Specified, STA sheet & plate
|
Tensile Strength, ksi |
0.2% Yield Strength, ksi |
Elongation in 2″, % |
|
170 |
160 |
10 |
| Regular shape for all kinds of alloys | |||
| Form | Specification | Supply Form | Others |
| Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
| Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
| Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
| Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
| Forged barΦ26-245mm,Length≤4000mm | |||
| Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
| Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
| Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
| Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
| Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
| Straight WireΦ1.6mm-4.0mm | |||
| Welding rodΦ1.2mm-4.0mm | |||
| Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Qingdao NPA Marketplace Co. Ltd is a foremost manufacturer specialized in centrifugal casting tube and static castings of warmth resistant alloys, which include ethylene cracking furnace tube, reformer furnace tube, CAL(constant annealing traces) &CGL(constant galvanizing traces) furnace roller and radiant tube, glass lehr roller and warmth/have on resistant castings. The annual potential is 9000 tons centrifugal casting tube and 3500 tons static castings (500 tons precision castings).
Internet site: www.npa-china.com
Melting down 1 gram bars of Silver, Copper, Nickel and Brass with hydrogen and oxygen. Brass is previously an alloy of copper and zinc, and did not soften down effortless as a I figured out from my Brass, Guide and Gunpowder video clip. I then blend the a few workable metals Silver, copper and nickel to generate…….Silvcopickel
SUBSCRIBE: http://comprehensive.sc/1bnslc9
Facebook: http://comprehensive.sc/1dT2aaM
RHNB Vs. Watermelon – http://comprehensive.sc/1bns60F
RHNB Vs. Jello – http://comprehensive.s/1bns0WF RHNB Vs. Elmers Glue – http://comprehensive.sc/1dT1TEM
RHNB Entire Playlist – http://comprehensive.sc/1dT1WjP -Want to ship an object / materials / substance to be RHNB’d or HHO’d? Send Here with a comprehensive credit of your donation! PO Box 21 96 Seymour St. Tonawanda NY 14150 Usa