OEM/ODM Supplier for Titanium alloy 10V-2Fe-3Al UNS R56410 for New Orleans Factories
To be the stage of realizing dreams of our employees! To build a happier, more united and more professional team! To reach a mutual benefit of our customers, suppliers, the society and ourselves for OEM/ODM Supplier for Titanium alloy 10V-2Fe-3Al UNS R56410 for New Orleans Factories, Adhering to the business principle of mutual benefits, we have won good reputation among our customers because of our perfect services, quality products and competitive prices. We warmly welcome customers from home and abroad to cooperate with us for common success.
HY Titanium 10-2-3 Material grades and equivalents
10-2-3 Titanium, UNS R56410
Introduction
HY Titanium 10-2-3 is a near beta alloy developed as a high strength forging alloy. This grade provides the best combination of strength and toughness of the commercially available titanium alloys. Its strength permits about a 27% weight savings when compared to Ti-6Al-4V. At the 180 ksi tensile strength level, the K1cvalue is 40 ksi-in ½ minimum. Solution treated and aged material possesses excellent resistance to stress corrosion cracking, typically K1scc being greater than 0.8 K1c. Solution treated material should not be subject to long term exposure in the 500-800°F range. This could result in high strength but low ductility.
High strength condition: Solution treat 60-100°F below the beta transus (typically 1460-1480°F), not less than 30 minutes, water quench. Age 900-975°F not less than 8 hours, air cool. For lower strength, overage in the 950-1150°F range. This alloy is deep hardenable, capable of high strengths in sections up to approximately 4″ thick.
This grade is usually supplied as billet or bar, finish rolled or forged in the alpha-beta field. For the high strength condition, the forging is usually given a pre-form forge above the beta transus, followed by 15-25% reduction below the beta transus.
Chemistry Composition
|
|
V |
Al |
Fe |
C |
N |
O |
H |
Y |
Others, |
Others, |
Ti |
|
MIN |
9.0 |
2.6 |
1.6 |
- |
- |
- |
- |
- |
- |
- |
- |
|
MAX |
11.0 |
3.4 |
2.22 |
0.05 |
0.05 |
0.13 |
0.015 |
0.005 |
0.10 |
0.30 |
Balance |
Features
- High strength and toughness
- Weight savings when compared to Ti-6Al-4V
- Excellent resistance to stress corrosion cracking
Applications
- Hand and die forgings
- Aircraft landing gear
- Golf club driver faces
Physical Properties
Density: 0.168 lb/inch³
Nominal Beta Transus: 1470°F
Poisson’s ratio: 0.32
Thermal Expansion: 75-800°F, 5.4×10-6 in/in°F
Tensile Modulus: 15.9×106 psi
Modulus: 16.2×106 psi
* 70°F to indicated temperature.
Mechanical Properties
Minimum Mechanical Properties AMS 4984, solution treated and aged
|
Ultimate Tensile Strength, ksi |
173 |
|
Ultimate Tensile Strength, ksi |
160 |
|
0.2% Yield Strength, ksi |
4 |
|
Reduction of Area, % |
Report |
|
fracture toughness, k1C |
40 ksi |
AMS 4987, single solution heat treat & overage
|
Ultimate Tensile Strength, ksi |
140 |
|
0.2% Yield Strength, ksi |
130 |
|
Elongation, % |
8 |
|
Reduction of Area, % |
20 |
|
fracture toughness, k1C |
80 ksi |
| Regular shape for all kinds of alloys | |||
| Form | Specification | Supply Form | Others |
| Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
| Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
| Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
| Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
| Forged barΦ26-245mm,Length≤4000mm | |||
| Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
| Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
| Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
| Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
| Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
| Straight WireΦ1.6mm-4.0mm | |||
| Welding rodΦ1.2mm-4.0mm | |||
| Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Qingdao NPA Marketplace Co. Ltd is a foremost manufacturer specialized in centrifugal casting tube and static castings of warmth resistant alloys, which include ethylene cracking furnace tube, reformer furnace tube, CAL(constant annealing traces) &CGL(constant galvanizing traces) furnace roller and radiant tube, glass lehr roller and warmth/have on resistant castings. The annual potential is 9000 tons centrifugal casting tube and 3500 tons static castings (500 tons precision castings).
Internet site: www.npa-china.com
Supplier foil、strip、sheet、coil、plate、wire、rod、bar、tube、pipe、flat ribbon、Profiled wire…
BuildingNo.1,3rd Industrial District XiTou Village SongGang Town Bao’An District ShenZhen Town GuangDong Province China