Online Manufacturer for Nickel Alloy Incoloy 901 UNS N09901 Wholesale to Karachi
Our eternal pursuits are the attitude of "regard the market, regard the custom, regard the science" and the theory of "quality the basic, trust the first and management the advanced" for Online Manufacturer for Nickel Alloy Incoloy 901 UNS N09901 Wholesale to Karachi, We welcome you to inquire us by call or mail and hope to build a successful and cooperative relationship.
HY 901 Material grades and equivalents
Incoloy 901/ Alloy 901/USN N09901/W.Nr.2.466 NS/BS Nimonic901
HY 901 (UNS N09901/Din 1.4898)
HY 901 Chemical composition:
|
Alloy |
% |
Ni |
Cu |
Al |
Fe |
Ti |
Co |
Mn |
S |
C |
Si |
P |
Cr |
Mo |
B |
|
HY 901 |
Min. |
40.0 |
2.35 |
11.0 |
5.0 |
0.01 |
|||||||||
|
Max. |
45.0 |
0.50 |
0.35 |
Balance |
3.10 |
1.0 |
1.0 |
0.03 |
0.10 |
0.60 |
0.03 |
14.0 |
7.0 |
0.02 |
HY 901 Physical properties:
|
Density |
8.14 g/cm3 |
|
Melting point |
1280-1345℃ |
HY 901 minimum mechanical properties in the room temperature:
|
Status |
Tensile strength |
Yield strength |
Elongation |
|
HY 901 |
1034 |
689 |
12 |
Description
A nickel-iron-chromium alloy containing titanium and aluminum for precipitation hardening and molybdenum for solid-solution strengthening. The alloy has high yield strength and creep resistance at temperatures to about 1110°F (600°C). A subtantial iron content enables the alloy to combine high strength with good forging characteristics. Used in gas turbines for discs and shafts. Standard products form is round.
Corrosion Resistance
Alloy 901 has good corrosion resistance to the atmospheres normally found in jet engine operations. It has slightly lower scaling resistance than such alloy as Types 309 and 310 stainless steel.
Workability
Hot Working
Alloy 901 is forged between 2050°F (1121°C) and 1850°F (1010°C), metal temperature. Light hot work may be continued down to 1600°F (871°C) but not below. Metal temperature should not exceed 2050°F (1121°C) during rapid working. Billets should be charged into a hot furnace and heated rapidly through the precipitation hardening range.
Weldability
Alloy 901 can be welded by the inert-gas-arc method. It is difficult to weld. All welding should be done in the solution treated condition. Cold worked parts should be re-solution treated before welding. A re-solution treatment is recommended after welding before stabilizing and aging.
| Regular shape for all kinds of alloys | |||
| Form | Specification | Supply Form | Others |
| Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
| Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
| Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
| Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
| Forged barΦ26-245mm,Length≤4000mm | |||
| Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
| Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
| Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
| Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
| Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
| Straight WireΦ1.6mm-4.0mm | |||
| Welding rodΦ1.2mm-4.0mm | |||
| Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
Visit my site for additional Recommendations, Films, Do it yourself assignments and additional:
http://www.mjlorton.com/
—————————–Click “Display additional”—————————————
A information on making use of the correct applications to crimp connectors, strip wire and implement warmth shrink.
You should guidance my information generation by making use of my Amazon Retail store:
http://astore.amazon.com/m0711-twenty
Purchase these applications and connectors below: http://astore.amazon.com/m0711-twenty?node=ten&site=one
——————— Click “Display additional” ——————————-
My site and forum:- http://www.mjlorton.com
Donations and contributions:- http://www.mjlorton.com
My techie channel MJLorton – Solar Power and Digital Measurement Products – http://www.youtube.com/MJLorton
My Techie Amazon Retail store: http://astore.amazon.com/m0711-twenty
My other channel VBlogMag – For nearly any matter beneath the sun! – http://www.youtube.com/VBlogMag
My VBlogMag Amazon Retail store: http://astore.amazon.com/vblogmag-twenty
———————————————————————–
=================================================
Online video sponsor, Pass Ltd – their internet websites:
http://www.tester.co.united kingdom/?cmid=QmhzQjcxYjVlc1E9&afid=bFcwbzliNzVDc289&ats=K2EyUjZNTDh3UTA9 – Examination Products and Examination-meter suppliers and
http://www.calibrate.co.united kingdom/?cmid=QmhzQjcxYjVlc1E9&afid=bFcwbzliNzVDc289&ats=S3Yxd2tOMjVISzA9 – Calibration and support of exam tools
=================================================
Additional dialogue and link to NASA information below:
http://mjlorton.com/forum/index.php?matter=244.
In this online video:
* Deciding upon the correct wire gauge (AWG – American Wire Gauge) for the crimp connector.
* Employing the correct applications to strip the insulation from the wire.
* The correct way to insert the wire into the crimp connector
* Employing the correct crimp applications to crimp the connector
* How to implement warmth shrink accurately to the wire and crimp connector.
Welding Inconel 718