Rapid Delivery for Titanium alloy 6Al-4V STA UNS R56400 Factory from Amman
We always think and practice corresponding to the change of circumstance, and grow up. We aim at the achievement of a richer mind and body and the living for Rapid Delivery for Titanium alloy 6Al-4V STA UNS R56400 Factory from Amman, We are sincere and open. We look forward to your visit and establishing trustworthy and long-term standing relationship.
HY Titanium 6-4 STA Material grades and equivalents
6-4 STA Titanium, 6-4 STA, Ti 6-4 STA, UNS R56400
Introduction
HY Titanium 6-4 STA (Solution Treated and Aged) is a modified version of Ti 6Al-4V. It is heat treated for high strength in sections under 4″ thick. Ti-6Al-4V has excellent hardenability in sections up to 1″ thick with strengths as high as 165 ksi.
For maximum strength: solution-treated and aged (STA) condition is: For sheet, 1675-1725°F 5 to 25 minutes, water quench. Age 975°F 4 to 6 hours, air cool. For bars and forgings, 1675-1725°F 1 hour, water quench. Age 975-1025°F 4 to 8 hours, air cool.
HY Titanium 6-4 STA is resistant to general corrosion but may be quickly attacked by environments that cause breakdown of the protective oxide. These include hydrofluoric (HF), hydrochloric (HCl), sulfuric and phosphoric acids. Inhibitors may help for the last three but not for HF. Ti 6Al-4V STA resists attack by pure hydrocarbons, and most chlorinated and fluorinated hydrocarbons (provided water has not caused formation of small amounts of HCl and HF).
Chemistry Composition
|
Al |
V |
C |
N |
O |
H |
Fe |
Y |
Others, |
Others, |
Ti |
|
|
MIN |
5.5 |
3.5 |
– |
– |
– |
– |
– |
– |
– |
– |
– |
|
MAX |
6.75 |
4.5 |
0.08 |
0.05 |
0.2 |
0.0125 |
0.3 |
0.005 |
0.1 |
0.4 |
Balance |
Features
High strength to 750°FExcellent general corrosion resistanceHigh strength-to-weight ratio
Applications
Aerospace, turbine engine and airframe applicationsFastenersMedical and dental implantsHigh performance Automotive
Physical Properties
Density: 0.160 lb/inch3
Melting Range: 2920 – 3020°F
Beta Transus: 1825± 25°F
|
Temperature, °F |
70 |
200 |
400 |
600 |
|
Coefficient of Thermal Expansion, in/in°F x 10-6 |
- |
5.3 |
5.4 |
5.5 |
|
Thermal Conductivity, |
4.0 |
4.3 |
5.2 |
6.1 |
|
Modulus of Elasticity, |
16.7 |
16.0 |
15.0 |
14.0 |
Mechanical Properties
Specified, STA sheet & plate
|
Tensile Strength, ksi |
0.2% Yield Strength, ksi |
Elongation in 2″, % |
|
170 |
160 |
10 |
| Regular shape for all kinds of alloys | |||
| Form | Specification | Supply Form | Others |
| Sheet | Thickness:0.40-4.75mm,General Width:1000、1219、1500mm | Whole Coil or piece of it | Cold Annealed,Surface 2B、2E |
| Plate | Thickness:4.76-60mm,Width:1500、2000、2500mm,Length:3000、6000、8000、8500mm(Under 10mm plate can be coiled) | Whole Coil or piece of it | Single hot rolling,Solid solution annealed state,Surface 1D |
| Belt | Thickness:0.10-3.0mm,Width:50-500mm | Whole Coil or Specified size | Cold Annealed,Surface 2B、2E |
| Bar & Rod | Rolled barΦ5-45mm,Length≤1500mm | Polished Bar(circle、Square) | Solution annealing,descaling |
| Forged barΦ26-245mm,Length≤4000mm | |||
| Weld tube | Outer diameterΦ4.76-135mm,Wall Thickness0.25-4.00mm,Length:≤35000 mm | Base on your requirement | |
| Seamless Tube | Outer diameterΦ3-114mm,Wall Thickness0.2-4.5mm | Base on your requirement | |
| Wire | Outer diameterΦ0.1-13mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Forged piece | discs,rings,squares,blocks,slabs | Base on your requirement | Steel, Alloy |
| Flangs | All kinds of Flangs | Base on your requirement | Steel, Alloy |
| Welding Material | Coil wire Φ0.025mm-1.6mm | Base on your requirement | Certificate of Origin:America, Sweden, Britain, Germany, Austria, Italy, France. |
| Straight WireΦ1.6mm-4.0mm | |||
| Welding rodΦ1.2mm-4.0mm | |||
| Tube | Elbow, three links, four links, different diameter size | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
| Explosive bonded laminate | Raw Sheet Thickness≥2mm | Base on your requirement | Ni & Ni alloy, Ti & Ti alloy |
http://www.weldingtipsandtricks.com/metals-and-how-to-weld-nickel.html
How to weld nickel alloys like hastelloy, inconel, etc. Nickel alloys have a low thermal conductivity and so limiting heat input and using lower amperage than would be used for stainless is one key to making good nickel alloy welds.